63Sn 37Pb
|
PROPERTY |
@300K |
UNITS |
REFERENCE |
|
Density |
8.41 |
G/cm3 |
14.1.A-B |
|
Specific Heat |
0.0358 |
Cal/g-k |
14.2.A-B |
|
Thermal conductivity |
0.119 |
Cal/cm-s-k |
14.3.A-D |
|
Thermal Expansion |
24x10-6 |
1/K |
14.4.A-C |
|
Melting Point |
456 |
K |
14.5.A-C |
|
Resistivity |
14.5x10-6 |
Ohm-cm |
14.6.A-C |
|
TCR |
4500 |
Ppm/K |
14.7.A |
|
Young’s Modulus |
4460 |
ksi |
14.8.A-C |
|
Poisson’s Ratio |
0.4 |
------ |
14.9.A |
|
Yield Strength |
4500 |
psi |
14.10.A |
|
Ult Tensile strength |
6360 |
psi |
14.11.A-F |
|
Elongation at break |
50 |
% |
14.12.A-C |
|
Hardness |
16 |
Vickers |
14.13.A-B |